国际标准成份 Chemical Specifications of Standards | ||||||||
元素 Element | Zamak 2 (%) | Zamak 3 (%) | Zamak 4 (%) | Zamak 5 (%) | Zamak 7 (%) | ZA-8 (%) | ZA-12 (%) | |
铝 Aluminum | (Al) | 3.9-4.3 | 3.9-4.3 | 3.9-4.3 | 3.9-4.3 | 3.9-4.3 | 8.2-8.8 | 10.8-11.5 |
镁 Magnesium | (Mg) | 0.035-0.050 | 0.04-0.05 | 0.04-0.05 | 0.04-0.05 | 0.010-0.02 | 0.020-0.030 | 0.020-0.030 |
铜 Copper | (Cu) | 2.7-2.9 | 0.03 max | 0.3-0.5 | 0.75-1.1 | 0.03 max | 0.8-1.3 | 0.5-1.2 |
铅 Lead | (Pb) | 0.003 max | 0.003 max | 0.003 max | 0.003 max | 0.002 max | 0.005 max | 0.005 max |
镉 Cadmium | (Cd) | 0.003 max | 0.002 max | 0.002 max | 0.002 max | 0.002 max | 0.005 max | 0.005 max |
锡 Tin | (Sn) | 0.001 max | 0.001 max | 0.001 max | 0.001 max | 0.001 max | 0.002 max | 0.002 max |
铁 Iron | (Fe) | 0.020 max | 0.020 max | 0.020 max | 0.020 max | 0.020 max | 0.065 max | 0.065 max |
镍 Nickel | (Ni) | 0.001 max | 0.001 max | 0.001 max | 0.001 max | 0.005-0.020 | 0.001 max | 0.001 max |
锌 Zinc | (Zn) | 余量 Balance | 余量 Balance | 余量 Balance | 余量 Balance | 余量 Balance | 余量 Balance | 余量 Balance |
Zamak3锌合金一向是压铸业的首选材料,它最能平衡物理和机械性能的要求。其优异的铸造性和尺寸持久稳定,使超过70%锌合金压铸产品都是用3号锌合金。Zamak3锌合金亦特别适合电镀、喷漆及铬化等表面处理。
Zamak3锌合金铸造性和尺寸持久稳定,使超过70%锌合金压铸产品都是用Zamak3锌合金。Zamak3锌合金电镀、喷漆及铬化等表面处理。产品广泛应用于汽车、摩托车、电子通讯、仪表等机械零件;以及玩具、饰物、餐具,锁类等高级五金器件。
使用过程中须注意的问题:
1. 抗蚀性差。当合金成分中杂质元素铅、镉、锡超过标准时,导致铸件老化而发生变形,表现为体积胀大,机械性能特别是塑性显着下降,时间长了甚至破裂。
铅、锡、镉在锌合金中溶解度很小,因而集中于晶粒边界而成为阴极,富铝的固溶体成为阳极,在水蒸气(电解质)存在的条件下,促成晶间电化学腐蚀。压铸件因晶间腐蚀而老化。
2. 时效作用
锌合金的组织主要由含Al和Cu的富锌固溶体和含Zn的富Al固溶体所组成,它们的溶解度随温度的下降而降低。但由于压铸件的凝固速度极快,因此到室温时,固溶体的溶解度是大大地饱和了。经过一定时间之后,这种过饱和现象会逐渐解除,而使铸件地形状和尺寸略起变化。
3. 锌合金压铸件不宜在高温和低温(0℃以下)的工作环境下使用。锌合金在常温下有较好的机械性能。但在高温下抗拉强度和低温下冲击性能都显着下降。
Zamak3锌合金质量保证, 公司以质量求生存,以信誉求发展,以科技求创新,保证产品质优价廉。以良好的售后服务热忱欢迎广大新老客户建立业务关系,携手合作欢迎咨询洽谈。
ZAMAK5号锌合金比3号锌合金的硬度和强度高,但柔软性较低,
如铸件须要折、屈、卷、锅等变形工序时可能有影响。5号锌合金的特性转变是由于加入了1%的铜,此合金铸造性优异,对抗蠕变(高温受力时变形)较3号锌合金好,同样适合电镀、切削加工及一般表面处理。
注:因价格浮动较大,故来电咨询价格为准!联系咨询:15121100374/021-56457673或者QQ联系:2463257819